PDF p. 1711 · 9-17
- 1.Base material reconditioning (sanding)
- -1.
Replacement part.
Lightly sand both sides of the part.
- -2.
Slight scores or scratches.
Use a flexible sanding block and wet-sand the damaged section with #400, #600.
NOTE: Sand level to remove damage.
- -3.
Deep scratches, when filling.
Use a flexible sanding block and wet-sand the damaged section with #400, #600.
- -1.
NOTE: Perform the featheredge on the material surface and coat surface (primer, intermediate coat and top coat) thoroughly and properly).
- Polish the levelled area with #400 sandpaper
- 2.
Degreasing/Cleaning
Clean the repair area with wax and grease remover, then blow dry with air.
NOTE: Wipe dust off the surface with a tack cloth.
- 3.Primer application
- Apply to the deep scratches and areas to be filled. This procedure might not be required by some manufacturer’s products.
- Spray wider than the damaged section (i.e. area to be filled) two to three times.
NOTE: Follow the manufacturer’s specifications.
- 4.
Coating with primer surfacer and drying
NOTE: Some manufacturer’s might require puttying before performing this step.
Spray the primer surfacer wider than the filled area and the exposed base material.
The spray guideline should be 20 - 23 microns.
NOTE: Follow the manufacturer’s instructions.
- After coating with the primer surfacer, let the primer surfacer dry naturally for 5 to 10 minutes, then dry the paint film of the primer surfacer with an infra-red dryer.
- When drying the primer surface with the dryer, be sure to keep the dryer 40 - 50 cm (16 - 20in) away from the paint film.
- 5.Filling, drying and sanding
- The exposed base material could be directly filled, depending on the manufacturer’s specification.
- Be sure that the primer surfacer is completely dry.
- Lightly dry sand the primer surfacer paint film with the #240 paper.
PDF p. 1712 · 9-18
- Apply the filler in several thin coats.
NOTE: Mix and apply the filler according to the manufacturer’s instructions.
- Dry the filler with an infra-red dryer for 5 to 6 minutes.
- While drying the filler with the dryer, be sure to keep the dryer 40 -50 cm (16 - 20 in) away from the surface.
- Scratch the filled surface with your nail. If the surface is white when scratched, dry sand and wet sand with the #280, #320 paper. Be sure to sand level.
- 6.
Cleaning with compressed air and degreasing
Blow the entire area that is to be coated with primer surfacer, with compressed air then clean with wax and grease remover.
NOTE: Also wipe the masking area to help the masking tape adhere securely.
- 7.
Masking
♦. Mask the area that should not be sprayed with the
primer surfacer.
- Use the masking tape and paper to mask.
- 8.
Coating with primer surfacer and drying
♦. Spray the two primer surfacer over the filled area.
- The spray guideline should be 20 - 25 microns.
NOTE: Follow the primer surfacer manufacturer’s instructions.
- After coating with the primer surfacer, let the primer surfacer dry naturally for 5 to 10 minutes, then dry with an infra-red dryer.
- While drying with the dryer, be sure to keep the dryer 40 -50 cm (16 - 20 in) away from the paint film.
- 9.
Sanding and cleaning
Lightly wet-sand the whole area to be painted with #600 sandpaper. Blow off with compressed air, then clean with wax and grease remover.
- 10.Top coating
- Remove dust with a tack cloth before top coating.
Spray the top coat paint.
Spray until the primer surfacer is covered. The spray guideline should be 30 -35 microns.
NOTE: For the recommended top coat paint, refer to the “4 Top coat” of “Example of repair materials”.
| Solid: | Colour enamel + colour clear coat. |
| Metallic: | Metallic enamel + clear coat. |
| Pearl: | Pearl enamel + clear coat. |
- 11.
Drying
After top coating about 10 minutes, dry with an infra-red dryer.
NOTE: Follow the paint manufacturer’s specification to dry properly.