Workshop manual

UP Resin Parts

Repair Procedures

Body Repair Manual 1999 · source: HRV_Workshop_Manual.pdf, PDF page 1710 (manual page 9-16)

PDF p. 1710 · 9-16

Illustration: SHALLOW SCRATCH: 1mm (0.04 in) approx.; DEEP SCRATCH: 2mm (0.08 in) approx.
  1. 1. SHALLOW SCRATCH: 1mm (0.04 in) approx.
  2. 2. DEEP SCRATCH: 2mm (0.08 in) approx.
  1. A.
    Replacement part:
    1. 1.
      Apply intermediate coat (grey). Sand both sides of the part (#400, #600).
    2. 2.
      Dry primer surfacer, then sand (#400, #600).
    3. 3.
      Apply top coating.
      1. -1.
        Metallic enamel + colour clear coat.
      2. -2.
        Solid colour enamel + clear coat.
      3. -3.
        Pearl enamel + clear coat.

NOTE: Also applicable to “Shallow scratches”, “Deep scratches” and “When filling”.

  1. B.

    Shallow scratch:

    Not down to the base material.

    1. 1.
      Sand top coat (#400, #600).
    2. 2.
      Apply top coating.
  1. C.
    Deep scratch, when filling:
    1. 1.
      Sand the damaged section (#180, #240).
    2. 2.
      Spray with primer and dry.

NOTE: When the base material is exposed.

  1. 3.
    Coat with primer surfacer.
  2. 4.
    Dry primer surfacer, then sand (#240, #400).
  3. 5.
    Apply polyester resin filler.
  4. 6.
    Dry polyester resin filler, then sand (#240, #320).
  5. 7.
    Coat with primer surfacer.
  6. 8.
    Dry primer surfacer, then sand (#400, #600).
  7. 9.
    Apply top coating.

NOTE: Coat with primer surfacer when the base material is exposed.